Na3Zr2Si2PO12 Ceramic Electrolytes rau Na-ion roj teeb: Kev npaj siv cov tshuaj tsuag kom qhuav thiab nws cov khoom
Tus sau:Li Wenkai, ZHAO Ning, BI Zhijie, GUO Xiangxin. Na3Zr2Si2PO12 Ceramic Electrolytes rau Na-ion roj teeb: Kev npaj siv cov tshuaj tsuag kom qhuav thiab nws cov khoom. Phau ntawv Journal of Inorganic Materials, 2022, 37(2): 189-196 DOI:10.15541/jim20210486
Abstract
Na-ion roj teeb, uas tam sim no siv cov nplaim hluav taws thiab tawg cov organic electrolytes, tam sim no ceev ceev yuav tsum tau tsim kom muaj kev ua tau zoo ntawm sodium ion khoom electrolyte kom paub ntau yam kev nyab xeeb thiab siv tau. Na3Zr2Si2PO12 yog ib qho kev cog lus zoo tshaj plaws sodium electrolytes rau nws qhov dav electrochemical qhov rais, siab mechanical zog, superior huab cua stability thiab siab ionic conductivity. Tab sis nws cov inhomogeneous sib xyaw ntawm cov ceramic hais nrog cov binders ua rau ntau qhov pores hauv lub cev ntsuab ua rau nws nyuaj kom tau txais high-density thiab high-conductivity ceramic electrolytes tom qab sintering. Ntawm no, txoj kev tshuaj tsuag kom qhuav tau siv los ua kom Na3Zr2Si2PO12 cov khoom sib xyaw ua ke nrog cov binders thiab granulated rau hauv cov khoom sib txuas. Raws li npaj ib txwm faib cov khoom tuaj yeem sib cuag tau zoo thiab txo qhov porosity ntawm ceramic ntsuab lub cev. Tom qab sintering, Na3Zr2Si2PO12 ceramic pellets ntawm cov tshuaj tsuag kom qhuav qhia cov txheeb ze ntawm 97.5% thiab ionic conductivity ntawm 6.96 × 10-4 S∙cm-1 ntawm chav tsev kub. Nyob rau hauv sib piv, tus txheeb ze ceev thiab chav-kub ionic-conductivity ntawm Na3Zr2Si2PO12 ceramic pellets npaj yam tsis muaj tshuaj tsuag-qhuav tsuas yog 88.1% thiab 4.94 × 10-4 S∙cm-1, raws li.
Ntsiab lus:khoom electrolyte; txoj kev tshuaj tsuag kom qhuav; ceev; ionic conductivity; Na3Zr2Si2PO12
Sodium ions thiab lithium ions ob leeg koom nrog thawj pab pawg, muaj cov tshuaj lom neeg zoo sib xws thiab cov txheej txheem sib txuas, thiab muaj kev nplua nuj nyob hauv cov peev txheej. Yog li ntawd, cov roj teeb sodium ion tuaj yeem ntxiv cov roj teeb lithium ion[1, 2, 3]. Sodium-ion roj teeb uas muaj cov nplaim taws, tsis muaj zog ntawm cov organic electrolytes tam sim no muaj kev txhawj xeeb txog kev nyab xeeb thiab tsis muaj zog txaus. Yog tias cov khoom siv electrolytes siv los hloov cov kua electrolytes, cov teeb meem kev nyab xeeb yuav tsum tau daws[4,5,6,7,8]. Inorganic khoom electrolytes muaj ib tug dav electrochemical qhov rais thiab yuav tsum matched nrog high-voltage cathode cov ntaub ntawv, yog li ua rau lub zog ceev ntawm cov roj teeb.[9]. Txawm li cas los xij, cov khoom siv electrolytes ntsib cov teeb meem xws li qis ionic conductivity thiab nyuaj ion kis tau tus mob ntawm qhov sib cuam tshuam ntawm electrodes thiab electrolytes. Thaum optimizing lub interface, nws yog thawj zaug yuav tsum nrhiav cov khoom electrolytes nrog siab ionic conductivity[10, 11, 12].
Tam sim no, feem ntau kawm sodium ion inorganic khoom electrolytes feem ntau muaj xws li Na- "-Al2O3, NASICON hom thiab sulfide. vim lawv lub qhov rais dav electrochemical, siab mechanical zog, stability rau huab cua, thiab siab ion conductivity [13,14]. Nws yog thawj zaug qhia los ntawm Goodenough thiab Hong li al.[15,16]. Cov mis mos dav dav yog Na{{0}}xZr2SixP3-xO12 (0 Tsawg dua lossis sib npaug rau x Tsawg dua lossis sib npaug rau 3), uas yog cov tshuaj txuas ntxiv tsim los ntawm NaZr2 (PO4)3 thiab Na4Zr2(SiO4)3 thiab muaj qhov qhib peb-dimensional Na+ kis tau tus mob channel. Na1+xZr2SixP3-xO12 muaj ob lub qauv: rhombus qauv (R-3c) thiab monoclinic qauv (C2/c, 1.8 Tsawg dua lossis sib npaug rau x Tsawg dua lossis sib npaug 2.2) . Thaum x=2, Na3Zr2Si2PO12 muaj qhov zoo tshaj plaws ionic conductivity. Ntawm 300 degree, ionic conductivity ntawm Na3Zr2Si2PO12 tuaj yeem ncav cuag 0.2 S∙cm-1, uas yog ze rau ionic conductivity ntawm Na-"-Al2O3 (0.1 ~ 0.3 S∙ cm -1) [15]. Tam sim no chav tsev kub ion conductivity ntawm Na3Zr2Si2PO12 qhia nyob rau hauv cov ntaub ntawv [17,18]yog kwv yees li ~10-4 S∙cm-1. Cov txheej txheem doping feem ntau yog siv los txhim kho ion conductivity. Txij li thaum NASICON cov khoom electrolyte muaj lub cev pob txha qhib, nws tuaj yeem doped nrog ntau yam ntsiab lus. Piv txwv li, cov ntsiab lus uas hloov Zr4+ suav nrog Mg2+, Zn2+, Al3+, Sc3+, Y3+, La{ {8}}, Ti4+, Hf 4+, Nb5+, Ta5+, etc.[17, 18, 19, 20, 21, 22]. Cov hloov P5+ suav nrog Ge5+ thiab As 5+ [22]. Ntxiv nrog rau cov khoom siv doping, nce qhov ntom ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv kuj yog ib txoj hauv kev los txhim kho lawv cov ionic conductivity. Tsis ntev los no, Yang et al.[18]siv cov khoom siv doping ua ke nrog sintering nyob rau hauv ib qho chaw oxygen los ua kom muaj zog heev Na3.2+2xZr2-x ZnxSi2.2P0.8O12 (0 Tsawg dua lossis sib npaug rau x Tsawg dua lossis sib npaug rau 0.15). Thaum x=0.1, chav tsev kub ionic conductivity ncav cuag tus nqi siab tshaj (5.27 × 10-3 S∙cm-1). Kev npaj ntawm Na3Zr2Si2PO12 ceramic electrolyte muaj xws li: cov pa sintering (CS), kua theem sintering (LPS), spark plasma sintering (SPS), microwave sintering (MWS), thiab txias sintering txheej txheem (CSP)[18-21,23-29]. Ntawm lawv, Huang et al.[20] siv cov txheej txheem sintering los ua kom qhov ceev ntawm ceramics los ntawm doping Ga3+. Ceramic electrolyte nrog chav tsev kub siab dua ionic conductivity (1.06 × 10-3 S∙cm-1) thiab qis hluav taws xob conductivity (6.17 × 10-8 S∙cm-1) tau txais. ZHANG et al.[21] tau txais kev pom zoo sintering txoj kev los ntawm kev qhia cation La{{0}}. Qhov nruab nrab theem Na3La(PO4)2 yog tsim nyob rau hauv ciam teb, thiab ib tug Na3.3Zr1.7La0.3Si2PO12 ceramic ntawv nrog ib tug ceev li 99.6% yog tau. Qhov sib thooj ntawm chav sov ion conductivity tuaj yeem ncav cuag 3.4 × 10-3 S∙cm-1. WANG et al.[23] siv microwave sintering (MWS) kom tau Na3Zr2Si2PO12 ceramics nrog lub siab ceev ntawm 96% ntawm qhov qis sintering ntawm 850 degree thiab tsuas tuav rau 0.5 h, txo cov nqi sintering. Qhov tseem ceeb ntawm cov txheeb ze ntom ntom (rrelative), ionic conductivity (σt) thiab ua kom lub zog (Ea) ntawm ceramic electrolytes npaj los ntawm ntau txoj kev yog teev nyob rau hauv Table 1.
Table 1 Cov ntsiab lus tseem ceeb ntawm NASICON-hom cov ntaub ntawv rau kev sib txawv sintering
|
Txoj kev sintering |
Kev sib xyaw |
Sintering |
Sintering |
Sijhawm/h |
kwv yees /% |
st/(S∙cm-1) |
E/eV |
Ref. |
|
CSP |
Na3.256Mg0.128Zr1.872Si2PO12 |
140 |
Tsis muaj |
1 |
82.9 |
0.41´10-4 |
- |
[19] |
|
FH-CSP |
Na3Zr2Si2PO12 |
375 |
NaOH |
3 |
93 |
2.2´10-4 |
0.32 |
[24] |
|
LPS |
Na3Zr2Si2PO12 |
1150 |
NaF |
24 |
- |
1.7´10-3 |
0.28 |
[25] |
|
LPS |
Na3Zr2Si2PO12 |
900 |
Na3BO 3 |
10 |
93 |
1.4´10-3 |
- |
[26] |
|
LPS |
Na3Zr2Si2PO12 |
1175 |
Na3SiO3 |
10 |
93 |
1.45´10-3 |
- |
[27] |
|
SPS |
Na3.4Zr1.6Sc0.4Si2PO12 |
1100 |
KOHaq |
0.1 |
95 |
9.3´10-4 |
- |
[28] |
|
SPS |
Na3Zr2Si2PO12 |
1210 |
Tsis muaj |
0.5 |
97.0 |
1.7´10-3 |
0.28 |
[29] |
|
MWS |
Na3Zr2Si2PO12 |
850 |
Tsis muaj |
0.5 |
96 |
2.5´10-4 |
0.31 |
[23] |
|
CS |
Na3Zr2Si2PO12 |
1250 |
Tsis muaj |
16 |
71.4 |
1.7´10-4 |
0.36 |
[20] |
|
CS |
Na3.1Zr1.9Ga0.1Si2PO12 |
1250 |
Tsis muaj |
16 |
86.5 |
1.06´10-3 |
0.29 |
[20] |
|
CS |
Na3Zr2Si2PO12 |
1200 |
Tsis muaj |
24 |
87.6 |
6.7´10-4 |
0.353 |
[21] |
|
CS |
Na3.3Zr1.7La0.3Si2PO12 |
1200 |
Tsis muaj |
24 |
99.6 |
3.4´10-3 |
0.291 |
[21] |
|
CS |
Na3Zr2Si2PO12 |
1250 |
Tsis muaj |
- |
84.02 |
2.17´10-4 |
0.407 |
[18] |
|
O2-CS |
Na3.4Zr1.9Zn0.1Si2.2P0.8O12 |
1250 |
Tsis muaj |
- |
99.46 |
5.27´10-3 |
0.285 |
[18] |
|
CS |
Na3Zr2Si2PO12 |
1250 |
Tsis muaj |
6 |
88.1 |
4.94´10-4 |
0.34 |
Qhov haujlwm no |
|
SD-CS |
Na3Zr2Si2PO12 |
1250 |
Tsis muaj |
6 |
97.5 |
6.96´10-4 |
0.32 |
Qhov haujlwm no |
CS: pa sintering; SD: tshuaj tsuag kom qhuav; O2-CS: pa sintering hauv cov pa ntshiab; CSP: txias sintering txheej txheem; FH-CSP: fused hydroxide txias sintering txheej txheem; MWS: microwave sintering; LPS: kua-theem sintering; SPS: spark plasma sintering
Cov txheej txheem siv cov hmoov npaj los ntawm kev sintering ncaj qha los sib tov nrog cov ntaub ntawv los tsim cov hmoov av ceramic, thiab tom qab ntawd ua cov hmoov molding thiab kub-kub sintering kom tau cov ceramics.[30, 31, 32]. Txawm li cas los xij, thaum lub sij hawm sib tsoo thiab sib xyaw ua ke, vim tias tsis sib xws hauv lub cev ntsuab, muaj ntau qhov kev sib tiv thaiv kab mob ceramic, muaj ntau yam ntom ntom thiab cov ionic conductivity siab. Txau kom qhuav yog ib txoj kev ziab sai uas siv lub atomizer kom tawg cov slurry rau hauv cov tee dej thiab siv cua kub kom qhuav cov tee kom tau cov hmoov. Cov khoom ntawm cov hmoov npaj los ntawm cov tshuaj tsuag kom qhuav yog spherical, thiab cov binder tuaj yeem sib npaug sib npaug ntawm cov khoom.[33]. KOJ et al. [34] siv cov tshuaj tsuag kom qhuav ua ke nrog kub-kub sintering los ua ke cov khoom electrolyte Li1.3Al0.3Ti1.7SixP5(3-0.8x)O12 (LATSP) nrog rau chav tsev kub ionic conductivity. Thaum x=0.05, chav tsev kub ionic conductivity nce mus txog qhov siab tshaj plaws ntawm 1.053 × 10-4 S∙cm-1, thiab qhov compacted ceev yog 2.892 g∙cm-3, uas yog ze rau qhov theoretical ntom ntom ntawm LATSP ntawm 2.94 g∙cm-3. Nws tuaj yeem pom tias cov tshuaj tsuag kom qhuav muaj qee qhov zoo hauv kev txhim kho qhov ntom ntom thiab ionic conductivity ntawm ceramic electrolytes. Nyob rau hauv kev pom ntawm qhov zoo ntawm cov tshuaj tsuag kom qhuav, cov nyhuv ntawm cov khoom doping ntawm ceramic ntom ntom thiab ionic conductivity yuav tsum raug txiav txim siab. Txoj kev tshawb no tau xaiv Na3Zr2Si2PO12 ua cov khoom tshawb fawb thiab qhia txog cov txheej txheem tshuaj tsuag granulation rau hauv kev npaj ua ntej ntawm cov ntaub ntawv hmoov los npaj Na3Zr2Si2PO12 ceramic electrolyte nrog high density thiab high ionic conductivity.
1 Kev sim txoj kev
1.1 Kev npaj khoom siv
Txoj kev npaj ntawm Na3Zr2Si2PO12 hmoov: Nyhav Na2CO3 (Aladdin, 99.99%), NH4H2PO4 (Aladdin, 99%), ZrO2 (Aladdin, 99.99%), thiab SiO2 (Aladdin, 99.99%) raws li stoichiometric ratio. Txhawm rau kom them nyiaj rau kev hloov pauv ntawm Na thiab P thaum lub sijhawm sintering, cov khoom siv raw muaj ntau tshaj 8% Na2CO3 thiab 15% tshaj ntawm NH4H2PO4. [25]. Zirconia npas tau siv los ua pob milling nruab nrab, cov khoom siv / pob qhov hnyav piv yog 1: 3, ethanol kiag li tau siv los ua qhov nruab nrab dispersion, thiab lub pob zeb siv rau pob milling rau 12 teev. Cov pob zeb-milled slurry tau qhuav hauv qhov cub ntawm 80 degree rau 12 teev. Cov hmoov qhuav yog av thiab dhau los ntawm 150 mesh (100 μm) sieve, thiab tom qab ntawd hloov mus rau 400 degree alumina crucible rau 2 h. Tshem tawm CO32- thiab NH{11}} los ntawm lub precursor, ces kub nws mus txog 1000 ~ 1150 degree rau calcination, thiab anneal nws tom qab 12 teev kom tau Na3Zr2Si2PO12 hmoov.
Txoj kev npaj ntawm Na3Zr2Si2PO12 cov nplooj ntawv ceramic: Txhawm rau tshawb xyuas cov txiaj ntsig ntawm Na3Zr2Si2PO12 particle loj ntawm qhov ntom ntom ntawm cov ntawv ceramic, ob pawg tswj kev sim tau tsim. Thawj pab pawg siv cov txheej txheem ib txwm siv, ntxiv 2% (feem ntau seem) polyvinyl cawv (Aladdin, Mw~205{{70}}00) binder rau theem ntshiab Na3Zr2Si2PO12 hmoov, ntxiv kiag li ethanol, thiab pob milling rau 12 teev. Cov hmoov tom qab pob milling yog qhuav, grinded thiab sieved kom tau ib tug hmoov coated nrog ib tug binder rau particle nto. Cov hmoov yog uniaxially txias nias ntawm 200 MPa siv lub stainless hlau pwm los ua ib lub cev ntsuab ntawm φ12 hli, kaw li GB. . Txhawm rau txo cov volatilization ntawm Na thiab P thaum lub sij hawm sintering txheej txheem ntawm ceramic los xij, lub cev ntsuab tau faus rau hauv niam hmoov thiab sintered ntawm 1250 degree rau 6 teev thiab tom qab ntawd annealed ntawm qhov kub ntawm 4 degree / min. Cov tau Na3Zr2Si2PO12 ceramic electrolyte tau raug xaiv los ua CS-NZSP. Cov pab pawg thib ob siv lub tshuab ziab khaub ncaws (ADL311S, Yamato, Nyiv) los ua granulate Na3Zr2Si2PO12 hmoov. Ntxiv 2% (loj feem) polyvinyl cawv (Aladdin, Mw ~ 205000) binder thiab 2% polyethylene glycol (Aladdin, Mn=1000) dispersant rau Na3Zr2Si2PO12 hmoov, thiab ntxiv ethanol kiag li. Npaj ib qho kev ncua nrog cov ntsiab lus ntawm 15% pawg pawg thiab pob zeb rau 12 teev. Lub pob-milled raug tshem tawm yog txau-qhuav nrog qhov ntsuas kub ntawm 130 degree thiab pub txaus tus nqi ntawm 5 mL / min. Na3Zr2Si2PO12 hmoov tau sau los ntawm lub tshuab hluav taws xob sib cais. Cov txheej txheem ntsiav tshuaj thiab ceramic sintering tau zoo ib yam li cov thawj pab pawg, thiab tau txais Na3Zr2Si2PO12 lub cev ntsuab thiab ceramic electrolyte tau sau tseg ua SD-GB thiab SD-CS-NZSP raws li. Kev kho deg polishing ntawm cov vuas ceramic: Ua ntej siv 400 mesh (38 μm) sanding daim ntawv rau ntxhib polishing, thiab tom qab ntawd siv 1200 mesh (2.1 μm) sanding ntawv rau polishing kom txog thaum lub ceramic nto du. Txoj kab uas hla ntawm CS-NZSP thiab SD-CS-NZSP ceramic electrolyte nplooj ntawv yog (11.3 ± 0.1) thiab (10.3 ± 0.1) hli feem, thiab lub thickness yog (1.0 ± 0.1) hli.
1.2 Lub cev yam ntxwv ntawm cov khoom
Kev soj ntsuam theem ntawm cov qauv tau ua los ntawm X-ray diffractometer (XRD, Bruker, D8 Advance). Qhov hluav taws xob qhov hluav taws xob yog CuK, lub raj siab yog 40 kV, lub raj ntws yog 40 mA, tus nqi luam tawm yog 2 (degree) / min, thiab qhov ntsuas ntsuas yog 2θ= 10 degree ~ 80 degree. Scanning electron microscope (SEM, Hitachi, S-4800) thiab kis tau tus mob electron microscope (TEM, JEOL, JEM-2100F) tau siv los tshuaj xyuas cov morphology ntawm cov qauv, thiab cov khoom siv EDX teeb tsa tau siv rau Elemental tsom xam.
1.3 Kev ntsuas hluav taws xob conductivity ntawm cov ntawv ceramic
Lub electrochemical impedance spectroscopy (EIS) ntawm tus qauv tau sim siv lub chaw ua haujlwm electrochemical. Qhov ntsuas zaus ntau yog 7 MHz ~ 0.1 Hz, qhov siv hluav taws xob yog 10 mV, qhov ntsuas nkhaus yog haum, thiab cov ionic conductivity ntawm cov khoom siv ceramic yog suav nrog cov qauv (1).
σ=L/(R×S) (1)
Hauv cov qauv, L yog qhov tuab ntawm daim ntawv ceramic (cm), R yog qhov tsis kam (Ω), S yog qhov thaiv electrode cheeb tsam (cm2), thiab σ yog ionic conductivity (S∙cm-1) .
Cov hluav taws xob conductivity ntawm cov qauv tau sim siv ncaj qha tam sim no polarization (DC), nrog rau qhov hluav taws xob tas li ntawm 5 V thiab lub sijhawm ntev ntawm 5000 s. Tus nqi ordinate tom qab qhov nkhaus yuav ruaj khov yog tus nqi tam sim no polarization. Siv cov qauv (2, 3) los xam cov hluav taws xob conductivity thiab sodium ion migration naj npawb ntawm daim ntawv ceramic.
σe=L×I/(V×S) (2)
t=(σ-σe)/σ (3)
Hauv cov qauv, L yog qhov tuab ntawm daim ntawv ceramic (cm), Kuv yog polarization tam sim no (A), V yog qhov voltage (V), S yog qhov thaiv electrode cheeb tsam (cm2), thiab σe yog cov hluav taws xob conductivity ( S∙cm-1). Txoj haujlwm no siv Au ua qhov thaiv electrode. Kev npaj ntawm thaiv electrode: Siv lub tshuab nqus tsev vacuum evaporation txheej cov cuab yeej siv siab (VZZ-300) kom evaporate qhov evaporation Au los ntawm cov cua kub tsis kam, thiab evaporate rau saum npoo ntawm daim ntawv ceramic. Daim ntawv ceramic yog tsau rau hauv ib lub ferrule nrog ib txoj kab uas hla ntawm 8 hli.
2 Cov txiaj ntsig thiab kev sib tham
2.1 Theem qauv thiab morphology characterization ntawm Na3Zr2Si2PO12
Txhawm rau ua kom zoo dua qhov kub ntawm sintering ntawm Na3Zr2Si2PO12, cov hmoov tau sintered ntawm 1000, 1050, 1100 thiab 1150 degree feem. X-ray diffraction qauv ntawm cov qauv tau txais nyob rau hauv txawv kub sintering yog qhia nyob rau hauv daim duab 1. Nws tuaj yeem pom los ntawm daim duab uas thaum lub sintering kub yog 1000 degree C, lub ntsiab theem ntawm Na3Zr2Si2PO12 tau tsim, tab sis muaj Na2ZrSi2O7. thiab ZrO2 impurity theem, thiab diffraction ncov siv ntawm lub ntsiab theem tsis muaj zog thiab ib nrab-ncej dav dav, qhia tau hais tias cov khoom sintering muaj tsis zoo crystallinity. Thaum lub sintering kub yog 1100 degree, lub ZrO2 impurity theem ploj mus thiab lub diffraction ncov siv ntawm lub Na2ZrSi2O7 impurity theem tsis muaj zog, qhia tau hais tias nce lub sintering kub yog zoo los tshem tawm cov impurity theem. Lub diffraction peaks ntawm cov khoom sintered ntawm 1100 thiab 1150 degree muaj me me ib nrab-ncej dav tshaj qhov diffraction peaks ntawm cov khoom sintered ntawm 1000 degree, qhia tias qhov siab dua qhov kub ntawm sintering, qhov zoo dua crystallinity ntawm cov khoom. Piv nrog rau 1000 degree sintered khoom, lub diffraction peaks ntawm 1150 degree sintered khoom yog phua ntawm 2θ=19.2 degree, 27.5 degree thiab 30.5 degree . Qhov no qhia tau hais tias cov khoom hloov pauv los ntawm theem rhombic nrog qis ionic conductivity mus rau theem monoclinic nrog siab ionic conductivity. [25,35]. Thiab lub ncov diffraction yog raws li tus qauv PDF 84-1200 diffraction ncov, qhia tias 1150 degree yog theem tsim kub ntawm Na3Zr2Si2PO12 khoom electrolyte nrog ib tug high ion conductivity monoclinic qauv.

Daim duab 1 XRD qauv ntawm Na3Zr2Si2PO12 hmoov sintered ntawm qhov kub thiab txias
Daim duab 2 qhia SEM duab thiab TEM cov duab ntawm Na3Zr2Si2PO12 hais tau los ntawm cov pa sib tov thiab tshuaj tsuag kom qhuav txoj kev. Daim duab 2(a) yog SEM daim duab ntawm Na3Zr2Si2PO12 hais tom qab sib xyaw ua ke. Nws tuaj yeem pom los ntawm daim duab tias cov duab ntawm cov khoom tsis sib xws, thiab txoj kab uas hla ntawm qee qhov hais txog 20 μm, qhia tias cov khoom tom qab sib xyaw ua ke yog qhov loj thiab tsis sib xws. Daim duab 2(b~c) qhia SEM duab ntawm Na3Zr2Si2PO12 hais tom qab tshuaj tsuag kom qhuav. Cov khoom yog spherical thiab particle txoj kab uas hla yog tsawg dua 5 μm, qhia tau hais tias cov particle zoo li niaj zaus thiab cov particle loj faib yog ntau concentrated tom qab tshuaj tsuag kom qhuav. Daim duab 2(d) yog daim duab TEM ntawm qhov chaw ntawm Na3Zr2Si2PO12 hais tom qab tshuaj tsuag kom qhuav. Particle nto yog tusyees coated nrog ib txheej ntawm binder nrog ib tug tuab ntawm txog 5 nm, uas yog conducive mus ze rau kev sib cuag ntawm ceramic hais.

Fig. 2 SEM cov duab ntawm Na3Zr2Si2PO12 particle tom qab sib xyaw ua ke (a) thiab tshuaj tsuag kom qhuav (bc), thiab TEM duab (d) ntawm Na3Zr2Si2PO12 particle nto tom qab txau kom qhuav
Daim duab 3 qhia txog qhov loj me me ntawm daim duab faib khoom ntawm polyvinyl cawv-coated Na3Zr2Si2PO12 (NZSP) tau los ntawm kev sib xyaw ua ke thiab polyvinyl cawv-coated Na3Zr2Si2PO12 (SD-NZSP) tau los ntawm txoj kev ziab kom qhuav. Nws tuaj yeem pom tau tias qhov ib nrab-ncej dav ntawm SD-NZSP particle loj faib nkhaus yog nqaim dua li ntawm NZSP particle loj nkhaus, qhia tias qhov loj me me faib tom qab cov tshuaj tsuag kom qhuav yog ntau concentrated. Qhov no yog qhov ua tau raws li cov txiaj ntsig tau pom hauv SEM cov duab hauv daim duab 2(a,b). Tsis tas li ntawd, qhov loj me me faib nkhaus tom qab ziab ziab yog ze rau qhov kev faib tawm ib txwm. Qhov no particle loj gradation tuaj yeem ua rau muaj kev sib cuag ntawm cov khoom thiab txo cov porosity ntawm lub cev ntsuab. Raws li qhia hauv Table 2, qhov ceev ntawm Na3Zr2Si2PO12 ntsuab lub cev npaj los ntawm cov qauv sib xyaw yog 83.01%, thiab qhov ceev ntawm Na3Zr2Si2PO12 ntsuab lub cev npaj los ntawm cov tshuaj tsuag kom qhuav yog nce mus rau 89.12%. Txhawm rau tshawb nrhiav ntxiv txog cov txiaj ntsig ntawm Na3Zr2Si2PO12 particle loj ntawm cov ceramic ntom ntom thiab conductivity, cross-sectional scanning, density ntsuas thiab conductivity test tau ua nyob rau ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv tau los ntawm cov pa sib tov thiab tshuaj tsuag kom qhuav txoj kev.

Daim duab 3 Na3Zr2Si2PO12 particle loj profiles ntawm cov pa sib xyaw (NZSP) thiab txau ziab (SD-NZSP) ntsuas los ntawm laser particle analyzer
Table 2 Sintering tsis thiab ntsuas qhov ceev thiab ntsuas tau ntawm Na3Zr2Si2PO12 khoom electrolyte ntsuab lub cev thiab ceramic ntawv
|
Qauv |
Txheej txheem temp./ degree |
Sijhawm/h |
m/g |
rethanol/(g·cm{0}}) |
msubmerged/g |
rreal/(g·cm-3) |
rtheoretical/(g·cm{0}}) |
kwv yees /% |
|
GB |
- |
- |
0.2902 |
0.785 |
0.2056 |
2.693 |
3.244 |
83.01 |
|
SD-GB |
- |
- |
0.2880 |
0.785 |
0.2098 |
2.891 |
3.244 |
89.12 |
|
CS-NZSP |
1250 |
6 |
0.2672 |
0.785 |
0.1938 |
2.858 |
3.244 |
88.10 |
|
SD-CS-NZSP |
1250 |
6 |
0.2644 |
0.785 |
0.1988 |
3.164 |
3.244 |
97.53 |
Daim duab 4 qhia txog daim duab ntawm lub cev ntawm Na3Zr2Si2PO12 ceramic daim ntawv, nws cov kab lus hla ntu morphology thiab cov duab tsom xam. Daim duab 4(a) qhia tau hais tias tus ntoo khaub lig-sectional morphology ntawm ceramic piece tau los ntawm cov pa sintering txoj kev. Nws tau pom tias muaj ntau qhov tsis sib xws hauv qhov hla ntawm daim ntawv ceramic, thiab lub pore hauv zos txoj kab uas hla tshaj 5 μm. Yog vim li cas yog qhov loj me me tom qab sib tsoo tsis sib xws, muaj cov khoom loj dua, thiab tsis muaj kev sib raug zoo ntawm cov khoom, uas ua rau cov pores tsis sib xws hauv cov ntawv ceramic thaum lub sij hawm thib ob sintering txheej txheem. Daim duab 4(b) qhia tau hais tias tus ntoo khaub lig-sectional morphology ntawm ceramic piece tau los ntawm cov tshuaj tsuag kom qhuav txoj kev. Cov pob zeb siv lead ua yog nyob ze rau ib leeg thiab tsis muaj qhov pom tseeb qhov hws. Qhov no qhia tau hais tias Na3Zr2Si2PO12 hais nrog cov duab tsis tu ncua thiab cov khoom siv loj me me tuaj yeem yooj yim tau txais cov nplooj ntawv ceramic thaum lub sij hawm sintering theem nrab. Qhov nce ntawm qhov ntom kuj tseem tshwm sim hauv qhov nce hauv qhov shrinkage ntawm lub cev ceramic tom qab sintering, raws li qhia hauv daim duab 4(c). Nyob rau sab laug yog ib daim ceramic tau los ntawm cov qauv sintering, nrog ib txoj kab uas hla ntawm 11.34 hli, thiab shrinkage tus nqi tsuas yog 5.5%; ntawm sab xis yog ib daim ceramic uas tau los ntawm txoj kev ziab kom qhuav, nrog txoj kab uas hla ntawm 10.36 hli, thiab qhov shrinkage ntawm 13.7%. Txhawm rau tshawb xyuas qhov muaj pes tsawg leeg ntawm txhua lub ntsiab lus hauv cov qauv, kev tshuaj xyuas cov ntsiab lus tau ua nyob rau ntawm ntu ntu ntawm cov khoom siv ceramic (Daim duab 4(b)), thiab daim duab 4 (d ~ g) tau txais. Cov ntsiab lus ntawm txhua lub ntsiab lus tau qhia nyob rau hauv Table 3. Txhua lub ntsiab lus tau muab faib ua tus sib npaug ntawm ntu ntu ntawm cov khoom siv ceramic, thiab tsis muaj cov khoom sib sau ua ke. Raws li Table 3, nws tau pom tias atomic feem pua ntawm Na thiab P yog 2.98: 1, uas yog ib txwm ua raws li tus qauv tshuaj formula ntawm Na: P=3: 1, qhia tias ntau tshaj Na thiab P hauv cov Cov khoom siv raw tuaj yeem them rov qab rau cov volatilization ntawm Na thiab P thaum lub sij hawm sintering.

Fig. 4 SEM cov duab ntawm cov ntawv hlais rau CS-NZSP (a) thiab SD-CS-NZSP (b), cov duab sib xws (c) thiab cov duab kos duab elemental (dg) ntawm SD-CS-NZSP
Table 3 Elemental tsom xam ntawm Na3Zr2Si2PO12 ceramic hlais ntu los ntawm cov tshuaj tsuag kom qhuav /%
|
Element |
O K |
Na K |
Si K |
P K |
Zr L |
|
Atomic feem pua |
60.10 |
15.09 |
9.94 |
5.06 |
9.81 |
|
Qhov hnyav feem pua |
36.43 |
13.13 |
10.59 |
5.94 |
33.91 |
2.2 Qhov ceev ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv
Qhov kev sim ntsuas qhov ntom ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv los ntawm Archimedes txoj kev[30].Txhawm rau kawm txog cov txiaj ntsig ntawm granulation txoj kev ntawm qhov ntom ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv, nyob rau hauv qhov kev sim tsis tau ntawm cov ntawv ceramic, cov kev sim ntsuas (sintering kub, tuav lub sijhawm, thiab lwm yam) ntawm pawg tswj kev sim tshwj tsis yog txoj kev granulation tau khaws cia. tib yam. Txhawm rau txo qhov cuam tshuam ntawm kev sim ntsuas qhov yuam kev ntawm qhov ntsuas qhov ntom ntom, qhov ntsuas qhov ntom tau rov ua dua ntawm cov qauv ntawm cov ntawv ceramic tau txais los ntawm txhua txoj kev npaj hauv qhov kev sim. Los ntawm kev sim cov ntaub ntawv qhia hauv Table 4, nws tuaj yeem pom tau tias qhov ntom ntawm CS-NZSP ceramic nplooj ntawv tau txais los ntawm cov qauv siv sintering yog 88.1%, uas yog qhov tseem ceeb raws li cov txiaj ntsig tau tshaj tawm hauv cov ntaub ntawv. [21].Qhov ceev ntawm SD-CS-NZSP ceramic nplooj ntawv tau los ntawm kev ziab kom qhuav tuaj yeem ncav cuag 97.5%, uas yog tus nqi siab tshaj tam sim no ua tiav los ntawm cov txheej txheem sintering tsis muaj cov khoom siv. Nws yog qhov siab dua li qhov ntom ntawm Na3Zr2Si2PO12 ceramic nplooj ntawv tau los ntawm lwm txoj kev sintering qhia hauv cov ntaub ntawv. Xws li txoj kev microwave sintering (96%)[23]Txoj kev txias sintering (93%)[24], kua theem sintering txoj kev (93%)[26] thiab tso tawm plasma sintering txoj kev (97.0%)[29].
Table 4 Ionic conductivity ntawm CS-NZSP thiab SD-CS-NZSP ntawm chav tsev kub
|
Qauv |
sb/(S·cm-1) |
sgb/(S·cm-1) |
st/(S·cm-1) |
E/eV |
|
CS-NZSP |
1.28×10-3 |
8.03×10-4 |
4.94×10-4 |
0.34 |
|
SD-CS-NZSP |
1.64×10-3 |
1.21×10-3 |
6.96×10-4 |
0.32 |
2.3 Na3Zr2Si2PO12 kev ntsuas hluav taws xob ua haujlwm
Daim duab 5(a) qhia txog chav tsev kub electrochemical impedance spectrum (EIS) ntawm cov ceramic wafer tau los ntawm cov qauv sintering thiab cov tshuaj tsuag kom qhuav. Lub semicircle nyob rau hauv daim duab qhia txog lub parallel impedance yam ntxwv ntawm grain ciam impedance thiab capacitive reactance. Qhov kev sib tshuam ntawm sab laug ntawm lub semicircle thiab abscissa sawv cev rau qhov tsis kam ntawm cov nplej. Lub ncua sij hawm ntawm lub semicircle ntawm lub abscissa qhia txog qhov tsis kam ntawm cov ciam teb, thiab oblique kab tom qab lub semicircle qhia txog impedance yam ntxwv ntawm thaiv electrode / electrolyte interface.[36]. Los ntawm kev haum rau EIS hauv daim duab 4, ionic conductivity ntawm CS-NZSP thiab SD-CS-NZSP tuaj yeem tau txais. Cov ntaub ntawv sim tau pom nyob rau hauv Table 4. Chav tsev kub ionic conductivity ntawm SD-CS-NZSP tau los ntawm cov tshuaj tsuag kom qhuav yog 6.96 ×10-4 S∙cm-1, uas siab dua li ntawm CS -NZSP (4.94 × 10-4 S∙cm-1) tau los ntawm txoj kev sintering pa. Los ntawm cov ntaub ntawv tsom xam ntawm EIS haum, nws tuaj yeem pom tias SD-CS-NZSP nrog cov qoob loo ntau dua thiab chav tsev kub siab dua.

Fig. 5 (a) EIS spectra ntawm chav tsev kub thiab (b) Arrhenius thaj av ntawm CS-NZSP thiab SD-CS-NZSP; (c) DC potentiostatic polarization tam sim no thiab (d) electrochemical qhov rais rau SD-CS-NZSP
Daim duab 5(b) qhia txog Arrhenius nkhaus ntawm chav tsev kub mus rau 100 degree rau cov nplooj ntawv ceramic tau los ntawm ntau txoj kev npaj. Nws tuaj yeem pom los ntawm daim duab uas lawv cov conductivity nce nrog nce kub. Thaum qhov kub nce mus txog 100 degree, qhov conductivity ntawm SD-CS-NZSP tuaj yeem ncav cuag 5.24 × 10-3 S∙cm-1, uas yog qhov kev txiav txim siab ntau dua li chav tsev kub conductivity. Nws lub zog ua kom haum raws li Arrhenius equationσ=Aexp(-Ea/kT)[7]. Kev ua kom muaj zog ntawm CS-NZSP thiab SD-CS-NZSP tau txais los ua 0.34 thiab 0.32 eV raws, uas zoo ib yam li daim ntawv tshaj tawm ntawm YANG li al.[18].
Cov khoom siv electrolyte yuav tsum muaj ob qho tib si siab ionic conductivity thiab qis hluav taws xob conductivity. Yog li ntawd, cov hluav taws xob conductivity ntawm SD-CS-NZSP tau ntsuas los ntawm qhov ncaj qha tam sim no polarization (DC), thiab qhov sib thooj polarization nkhaus yog qhia hauv daim duab 5(c). Nws tuaj yeem pom los ntawm daim duab tias raws li lub sijhawm ntsuas ncua ntev, cov polarization tam sim no maj mam txo qis; thaum lub sij hawm xeem mus txog 5000 s, lub polarization tam sim no (I=3.1 μA) tsis hloov lawm raws li lub sij hawm xeem ntev. Muab xam los ntawm cov qauv (2, 3), cov hluav taws xob conductivity ntawm SD-CS-NZSP yog 1.23 × 10-7 S∙cm-1, thiab cov sodium ion migration tooj yog 0.9998. Txoj kev tshawb no kuj ntsuas lub qhov rais electrochemical ntawm SD-CS-NZSP los ntawm cyclic voltammetry (CV)[18]. Raws li pom nyob rau hauv daim duab 5(d), ob oxidation thiab txo peaks tshwm nyob ib ncig ntawm 0 V, sawv cev rau stripping thiab deposition ntawm sodium feem.[20]. Ntxiv rau qhov no, tsis muaj lwm yam redox peaks tau pom nyob rau hauv qhov ntsuas hluav taws xob ntau. Qhov no txhais tau hais tias tsis muaj qhov hloov pauv tam sim no vim qhov decomposition ntawm cov electrolyte nyob rau hauv qhov hluav taws xob ntau ntawm 0~ 6 V, qhia tias SD-CS-NZSP muaj kev ruaj ntseg electrochemical zoo. Lub qhov rais dav electrochemical (6 V (vs. Na / Na +)) tuaj yeem phim cov sodium-ion khoom electrolyte rau cov khoom siv hluav taws xob cathode, xws li cov khoom siv nickel-manganese-based cathode, uas yog qhov zoo rau kev txhim kho lub zog ntom ntom ntawm sodium. - ion roj teeb.
3 Kev xaus
Ib txoj kev kub-kub-theem-theem tau siv los ua ke cov ntshiab-theem Na3Zr2Si2PO12 hmoov ntawm sintering kub ntawm 1150 degree los ntawm kev qhia ntau tshaj Na thiab P mus rau hauv lub precursor. Siv cov tshuaj tsuag kom qhuav rau spherically granulate cov hmoov, cov polyvinyl cawv binder yog uniformly coated rau saum npoo ntawm Na3Zr2Si2PO12 hais thiab particle loj tis yog ze rau ib txwm faib. Qhov ceev ntawm cov npaj Na3Zr2Si2PO12 ceramic nce mus txog 97.5%. Kev ua kom ceev tuaj yeem txo qis ciam teb tsis kam, thiab cov ionic conductivity nce mus txog 6.96 × 10-4 S∙cm-1 ntawm chav tsev kub, uas yog siab dua cov ntawv ceramic npaj los ntawm cov qauv sintering (4.94 × {{24). }} S∙cm-1). Tsis tas li ntawd, cov ceramics uas tsim los ntawm txoj kev ziab kom qhuav muaj lub qhov rai electrochemical dav dav (6 V (vs. Na / Na +)) thiab tuaj yeem sib xyaw nrog cov khoom siv hluav taws xob cathode kom nce lub zog ceev ntawm lub roj teeb. Nws tuaj yeem pom tau tias txoj kev txau ziab yog cov qauv siv ntom ntom ntom nti thiab yog qhov haum rau lwm hom ceramic khoom electrolytes.
Cov ntaub ntawv
[1] JIAN ZL, ZHAO L, Pan HL, et al. Cov pa roj carbon coated Na3V2 (PO4) 3 ua cov khoom siv electrode tshiab rau cov roj teeb sodium-ion. Electrochemistry Communications, 2012,14(1):86-89.
[2] ZHAO L, ZHAO JM, HU YS, et al. Disodium terephthalate (Na2C8H4O4) raws li kev ua haujlwm siab anode khoom rau cov nqi qis hauv chav tsev kub-kub sodium-ion roj teeb. Advanced Energy Materials, 2012,2(8):962-965.
[3] RUAN YL, GUO F, LIU JJ, et al. Optimization ntawm Na3Zr2Si2PO12 ceramic electrolyte thiab interface rau kev ua haujlwm siab-lub xeev sodium roj teeb. Ceramics International, 2019,45(2):1770-1776.
[4] VETTER J, NOVAK P, WAGNER MR, et al. Kev laus mechanisms hauv lithium-ion roj teeb. Phau ntawv Journal of Power Sources, 2005,147(1/2):269-281.
[5] KAMAYA N, HOMMA K, YAMKAWA Y, et al. Lithium superionic conductor. Nature Materials, 2011,10(9):682-686.
[6] TARASCON JM, ARMAND M. Cov teeb meem thiab cov teeb meem ntsib cov roj teeb lithium rechargeable. Xwm, 2001,414(6861):359-367.
[7] KHOKHAR WA, ZHAO N, Huang WL, et al. Kev coj cwj pwm sib txawv ntawm cov hlau nkag hauv Na thiab Li khoom electrolytes. ACS Applied Materials & Interfaces, 12(48):53781-53787.
[8] OUDENHOVEN JFM, BAGGETTO L, NOTTEN PH L. All- solid-state lithium-ion microbatteries: kev tshuaj xyuas ntawm ntau yam peb-seem ntsiab lus. Advanced Energy Materials, 2011,1(1):10-33.
[9] ZHAO CL, LIU LL, QI XG, et al. Solid-state sodium roj teeb. Advanced Energy Materials, 2017,8(17):1703012.
[10] HAYASHI A, NOI K, SAKUDA A, et al. Superionic iav-ceramic electrolytes rau chav-kub rechargeable sodium roj teeb. Nature Communications, 2012, 3:856.
[11] LOU SF, ZHANG F, FU CK, et al. Cov teeb meem cuam tshuam thiab cov teeb meem hauv cov roj teeb uas tsis muaj zog: lithium, sodium, thiab tshaj. Advanced Materials, 2020,33(6):2000721.
[12] Huang WL, ZHAO N, BI ZJ, et al. Peb puas tuaj yeem nrhiav kev daws kom tshem tawm Li nkag los ntawm cov khoom garnet electrolytes? Cov ntaub ntawv niaj hnub Nano, 2020, 10: 100075.
[13] JIAN ZL, HU YS, JI XL, et al. NASICON-structured cov ntaub ntawv rau lub zog cia. Advanced Materials, 2016,29(20):1601925.
[14] HOU WR, GUO XW, SHEN XY, et al. Cov khoom siv electrolytes thiab cuam tshuam hauv cov roj teeb uas muaj zog-lub xeev sodium: kev nce qib thiab kev pom. Nano Zog, 2018,52:279-291.
[15] GOODENOUGH JB, HONG HYP, KAFALAS JA. Ceev Na+-ion thauj hauv cov pob txha pob txha. Cov ntaub ntawv tshawb fawb cov ntawv xov xwm, 1976,11(2):203-220.
[16] HONG HY P. Cov qauv siv lead ua thiab siv lead ua chemistry hauv qhov system Na1+xZr2SixP3-xO12. Cov Ntaub Ntawv Tshawb Fawb, 1976,11(2):173-182.
[17] RAN LB, BAKTASH A, LI M, et al. Sc, Ge co-doping NASICON boosts solid-state sodium ion roj teeb 'kev ua tau zoo. Energy Storage Materials, 2021,40:282-291.
[18] Yang J, LIU GZ, AVDEEV M, et al. Ultrastable all-solid-state sodium rechargeable roj teeb. ACS Energy Letters, 2020,5(9):2835-2841.
[19] Leng HY, Huang JJ, NIE JY, et al. Txias sintering thiab ionic conductivity ntawm Na3.256Mg0.128Zr1.872Si2PO12 khoom electrolytes. Phau ntawv Journal of Power Sources, 2018,391:170-179.
[20] Huang CC, Yang GM, YU WH, et al. Gallium hloov Nasicon Na3Zr2Si2PO12 khoom electrolytes. Phau ntawv Journal of Alloys And Compounds, 2021,855:157501.
[21] Zhang ZJ, ZHANG QH, SHI JN, et al. Ib tug self-forming composite electrolyte rau solid-state sodium roj teeb nrog ultralong voj voog lub neej. Advanced Energy Materials, 2017,7(4):1601196.
[22] ANANTHARAMULU N, RAO KK, RAMBABU G, et al. Kev tshuaj xyuas dav dav ntawm Nasicon cov ntaub ntawv. Phau ntawv Journal of Materials Science, 2011,46(9):2821-2837.
[23] WANG XX, Liu ZH, TANG YH, et al. Tsawg kub thiab ceev microwave sintering ntawm Na3Zr2Si2PO12 khoom electrolytes rau Na-ion roj teeb. Phau ntawv Journal of Power Sources, 2021,481:228924.
[24] GRADY ZM, TSUJI K, NDAYISHIMIYE A, et al. Densification ntawm ib tug solid-state NASICON sodium-ion electrolyte hauv qab 400 degree los ntawm txias sintering nrog ib tug fused hydroxide hnyav. ACS Applied Energy Materials, 2020,3(5):4356-4366.
[25] Shao YJ, ZHONG GM, LU YX, et al. Ib qho tshiab NASICON-raws li iav-ceramic composite electrolyte nrog txhim kho Na-ion conductivity. Zog Cia Khoom, 2019,23:514-521.
[26] LENG HY, NIE JY, LUO J. Kev sib xyaw txias sintering thiab Bi2O3- ua kom cov kua-theem sintering los tsim cov khoom siv hluav taws xob siab Mg-doped NASICON ntawm qhov kub thiab txias. Phau ntawv Journal of Materiomics, 2019,5(2):237-246.
[27] OH JAS, HE LC, PLEWA A, et al. Composite NASICON (Na3Zr2Si2PO12) solid-state electrolyte nrog txhim kho Na + ionic conductivity: cov nyhuv ntawm cov kua theem sintering. ACS Applied Materials & Interfaces, 2019,11(43):40125-40133.
[28] DA SILVA JGP, BRAM M, LAPTEV AM, et al. Sintering ntawm sodium-raws li NASICON electrolyte: ib qho kev kawm sib piv ntawm txias, teb pab thiab cov pa sintering txoj kev. Phau ntawv Journal of the European Ceramic Society, 2019,39(8):2697-2702.
[29] WANG H, OKUBO K, INADA M, et al. Tsawg kub-densified NASICON-raws li ceramics txhawb los ntawm Na2O-Nb2O5-P2O5 iav additive thiab spark plasma sintering. Solid State Ionics, 2018,322:54-60.
[30] HUO HY, GAO J, ZHAO N, et al. Ib qho yooj yim electron-blocking interfacial shield rau dendrite-dawb cov khoom lithium hlau roj teeb. Nature Communications, 2021,12(1):176.
[31] JIA MY, ZHAO N, HUO HY, et al. Kev tshawb nrhiav dav rau hauv garnet electrolytes rau daim ntawv thov-oriented cov roj teeb lithium. Electrochemical Zog Xyuas, 2020,3(4):656-689.
[32] ZHAO N, KHOKHAR W, BI ZJ, et al. Khoom siv roj teeb garnet. Joule, 2019, 3(5):1190-1199.
[33] VERTRUYEN B, ESHRAGHI N, PIFFET C, et al. Txau-qhuav ntawm cov khoom siv electrode rau lithium- thiab sodium-ion roj teeb. Cov ntaub ntawv, 2018, 11(7): 1076.
[34] KOU ZY, MIAO C, Wang ZY, et al. Novel NASICON-type structural Li1.3Al0.3Ti1.7SixP5(3-0.8x)O12 khoom electrolytes nrog txhim kho ionic conductivity rau lithium ion roj teeb. Lub Xeev Ionics, 2019, 343: 115090.
[35] SHEN L, Yang J, Liu GZ, et al. High ionic conductivity thiab dendrite-resistant NASICON khoom electrolyte rau tag nrho cov-solid-state sodium roj teeb. Materials Today Zog, 2021, 20: 100691.
[36] Li YQ, WANG Z, Li CL, et al. Densification thiab ionic-kev txhim kho ntawm lithium garnet khoom electrolytes los ntawm ntws oxygen sintering. Phau ntawv Journal of Power Sources, 2014,248:642-646.